FIRST YEAR · CHEMISTRY · CHAPTER 5 OF 8

Electrochemistry: cells, batteries and corrosion

This chapter shows how two half-cells give an emf, how that emf is a free energy change and how concentration shifts it. The same ideas explain batteries, fuel cells and rusting, which an engineer needs to choose a cell and keep metal from corroding.

Updated 30 Oct 2026

What you will be able to do

You will find a cell's emf from two half-cell potentials and turn it into a free energy change. You will correct the emf for concentration. You will say what moves where in a lithium-ion cell and a fuel cell. You will explain why iron rusts and choose a way to protect it.

Before you start

  1. Chapter 3, Thermodynamics, free energy and equilibrium, including the reaction quotient and

  2. Logarithms to base 10 and natural logarithms

  3. Oxidation as loss and reduction as gain of electrons, and adding two half-reactions so the electrons cancel

Electrode potential and cell emf

A galvanic cell is two half-cells, each a metal in a solution of its own ions, joined by a wire and a salt bridge. A spontaneous reaction pushes electrons through the wire; ions crossing the bridge keep each solution neutral. Only differences can be measured, so the standard hydrogen electrode (SHE), platinum in 1 mol/L with at 1 bar, is set to 0 V.

A half-cell's electrode potential is its emf against the SHE, written as a reduction; is its value at 1 mol/L, 1 bar and, unless stated, 298 K. Potentials strictly depend on activities (effective concentrations); for dilute solutions this chapter takes them as concentrations in mol/L. Ordered by , they form the electrochemical series: under standard conditions, the more negative, the more readily the metal gives up electrons.

Couple (reduction)

at 298 K (V)

CELL EMF FROM TWO HALF-CELLS

Both are reduction potentials, in V. Oxidation happens at the anode, reduction at the cathode. A positive means the reaction runs as written under standard conditions.

FREE ENERGY AND CELL EMF

Constant and . This links to Chapter 3: is the most non-expansion work a change can do, and a cell drawing almost no current gives it all as electrical work, charge times . = moles of electrons per mole of reaction as written, C/mol, in V, in J/mol.

WATCH OUT FOR

Doubling a half-reaction does not double . Test: is energy per unit charge, independent of the amount reacting; doubles through .

WORKED EXAMPLE

A zinc rod in 1 mol/L is joined by a salt bridge to a copper rod in 1 mol/L at 298 K. Find the cell reaction, and .

Solution
  1. has the more positive , so takes electrons: copper is the cathode, zinc the anode.

  2. Adding and cancels two electrons: .

  3. V, positive, so the reaction runs as written.

  4. C/mol V J/mol (C V = J).

Answer: , V, kJ/mol.

Nernst equation, concentration cells and conductance

A working cell is not at 1 mol/L, and its emf changes as it runs. Start from Chapter 3, , and replace each free energy by .

NERNST EQUATION

Divide by . = reaction quotient of the cell reaction, solids left out, concentrations in mol/L; J/(mol K), in K; at 298 K, V. At equilibrium and .

EMF OF A CONCENTRATION CELL

At 298 K. One metal in solutions of its ion at two concentrations, so . It dissolves on the dilute side (anode) and plates out on the concentrated side (cathode): ions pass from concentrated to dilute, . in mol/L, in V.

Ions carry current through a solution. Its conductance is in siemens (S); its conductivity , in S/m, is the conductance between opposite faces of a 1 m cube. In dilute solutions falls on dilution (fewer ions per cubic metre), so electrolytes are compared per mole.

MOLAR CONDUCTIVITY

in S/m, in mol/m (1 mol/L = 1000 mol/m), in S m/mol.

rises on dilution. A strong electrolyte is almost fully dissociated: its ions, farther apart, attract each other less, so rises slowly to a limit. A weak electrolyte dissociates more as falls, so its rises steeply at low .

WORKED EXAMPLE

In the zinc-copper cell above, mol/L and mol/L at 298 K. Find the emf.

Solution
  1. The reaction is unchanged, so and V.

  2. Solids are left out of : .

  3. V.

  4. Little product ion means the reaction is further from equilibrium, so is above .

Answer: V.

Batteries and fuel cells

A battery is one or more galvanic cells in a case. On discharge the anode feeds electrons into the outside circuit, so it is the negative terminal. A primary cell, such as the alkaline cell (zinc and , about 1.5 V), cannot be recharged in practice. A secondary cell can: a charger drives current backwards and reverses the reaction, as in the lead-acid cell (Pb and , about 2.0 V) and the lithium-ion cell (about 3.7 V).

A lithium-ion cell holds no lithium metal. Lithium ions shuttle between graphite (negative) and lithium cobalt oxide (positive). On discharge they cross the electrolyte from graphite to oxide while electrons take the outside circuit the same way. On charge, the charger pushes electrons back to the graphite and the ions follow.

LITHIUM-ION CELL REACTION

Discharge left to right, charge right to left; . On discharge the graphite is oxidised () and the oxide reduced. stands for the oxide with lithium removed.

WATCH OUT FOR

On charge, is the graphite still the anode? Test: the anode is where oxidation happens. On charge that is the oxide, so the oxide is the anode; the negative and positive terminals stay the same.

A fuel cell is a galvanic cell fed with its reactants from outside, so it runs while fuel and air arrive. In the hydrogen-oxygen cell with an acid electrolyte, protons cross the electrolyte, electrons take the outside circuit, and water is the only chemical product.

HYDROGEN-OXYGEN FUEL CELL

Acid electrolyte, 298 K, liquid water. The oxygen half-reaction has V and the hydrogen one 0 V, so V. Per mole of , : J/mol kJ/mol.

Corrosion and its prevention

Wet corrosion is a galvanic cell on one piece of metal. The moisture film is the electrolyte and the metal carries electrons. Iron dissolves at anodic areas where oxygen is scarce (a drop's centre, a crevice, a pit); the cathode forms where oxygen arrives easily, such as the drop's rim.

RUSTING OF IRON

Moist iron in air. The oxygen half-reaction has V (1 mol/L ), so V. Air then oxidises to rust, , often away from the pit.

Corrosion speeds up with dissolved salts (sea water conducts better), more oxygen at the cathode, acid (a second cathode reaction, ), contact with a less active metal (iron joined to copper becomes the anode), strained or scratched metal and, usually, a higher temperature. The defences:

  1. Coatings: paint, oil or a metal plating keep water and air off.

  2. Sacrificial anode: a more active metal such as Mg or Zn, wired to the iron, becomes the anode and dissolves, so the iron stays the cathode. It is replaced when used up.

  3. Impressed current: a DC source, negative terminal on the structure and positive on a buried inert anode such as graphite, keeps the structure cathodic.

  4. Inhibitors: a little phosphate, nitrite or an amine in the liquid forms a film or blocks active spots.

WATCH OUT FOR

Zinc and tin both coat steel, but a scratch differs. Test: compare with iron's V. Zinc ( V) is more negative, so it is the anode and the steel is kept. Tin ( V) is not, so the exposed iron corrodes.

Check yourself

CHECK YOURSELF 1

At 298 K, values are: V, V, V, V, V. Which metal can be wired to an iron pipe as a sacrificial anode?

  1. (A)

    Copper

  2. (B)

    Silver

  3. (C)

    Tin

  4. (D)

    Magnesium

Answer and solution

Answer: (D)

  1. A sacrificial anode must be more active than iron: its must be more negative than V.

  2. Only magnesium ( V) qualifies. With copper, silver or tin, iron would be the anode.

  3. Answer: D.

CHECK YOURSELF 2

A cell is built from ( V) and ( V), both at 1 mol/L and 298 K. For the reaction , find in kJ/mol. Use C/mol.

Answer and solution

Answer: (accepted range )

  1. Silver is the cathode and iron the anode: V.

  2. Two electrons are transferred, so .

  3. J/mol kJ/mol.

CHECK YOURSELF 3One or more options are correct

A lithium-ion cell is being discharged. Which statements are true?

  1. (A)

    Lithium ions move through the electrolyte from the graphite to the oxide.

  2. (B)

    Electrons flow in the outside circuit from the graphite to the oxide.

  3. (C)

    Lithium ions move through the electrolyte from the oxide to the graphite.

  4. (D)

    The oxide electrode is the cathode.

Answer and solution

Answer: (A), (B), (D)

  1. On discharge, lithium leaves the graphite as and enters the oxide: A true, C false.

  2. The graphite is oxidised and its electrons travel round the outside circuit to the oxide: B true.

  3. Reduction occurs at the oxide, so it is the cathode: D true.

CHECK YOURSELF 4

A drop of salt water sits on a clean iron plate in air. Where does the iron mainly dissolve?

  1. (A)

    At the rim of the drop, where oxygen is plentiful

  2. (B)

    At the centre of the drop, where oxygen is scarce

  3. (C)

    Evenly over the whole wetted area

  4. (D)

    Only where the plate is scratched

Answer and solution

Answer: (B)

  1. Oxygen is reduced where it arrives easily, the rim, so the rim is cathodic.

  2. The anodic area, where iron dissolves, is the oxygen-poor centre.

  3. Answer: B.